TypeSpecimen numberUltimate load (kN)Rebar stress (MPa)Lower yield (kN)Yield strength (MPa)Slip (mm)Destruction mode

DGTZB16-PZ-BM-1115.76575.9284.76421.696.99Rebar tension fracture
GTZB16-PZ-BM-2114.28568.5682.80411.946.74Rebar tension fracture
GTZB16-PZ-BM-3114.28568.5687.41434.886.98Rebar tension fracture

AVGGTZB16-DZ-BM-AVG119.73595.6787.35434.597.32Rebar tension fracture