Research Article

Research and Model Prediction on the Performance of Recycled Brick Powder Foam Concrete

Table 8

Orthogonal test results of ordinary foam concrete.

Group numberDry density (kg/m3)28 d compressive strength (MPa)Specific strength (N·m·kg−1)Group numberDry density (kg/m3)28 d compressive strength (MPa)Specific strength (N·m·kg−1)

1743.552.2903079.8214591.61.1821997.97
2722.382.2293085.6315590.31.0141717.77
3707.61.9982823.6316644.11.7342692.13
4714.92.0122814.3817628.71.5482462.22
5639.41.6682608.7018584.10.9491624.72
6536.00.8801641.7919599.71.2122021.01
7735.22.1092868.6120550.30.9191670.00
8797.12.4083020.9521608.41.2292020.05
9648.60.8531315.1422500.10.8751749.65
10567.40.8301462.8123672.71.4622173.33
11713.81.6572321.3824592.81.0731810.05
12638.21.4712304.9225567.40.9511676.07
13615.91.6312648.16