Research Article
Study on Road Performance of Cement-Stabilized Recycled Aggregate Base with Fiber and Rubber
Table 2
Test results of properties of recycled coarse aggregate.
| Performance index | Apparent density (g/cm3) | Hygroscopic rate (%) | Bulk density (g/cm3) | Crush value (%) | Needle sheet content (%) | Mud content (%) | Clay lump content (%) |