Partial Replacement of Cement by Waste Paper Pulp Ash and Its Effect on Concrete Properties
Table 15
Compressive strength loss (CSL) of OPC-WPPA and PPC-WPPA concrete cured in 2% sulfuric acid solution.
| S. no. | Mix code | Average compressive strength before immersion in MPa | Average compressive strength after immersion in MPa | Compressive strength loss (CSL) in % |
| 1 | OPC-WPPA0 | 34.579 | 31.571 | 8.825 | 2 | OPC-WPPA5 | 36.827 | 33.586 | 8.424 | 3 | OPC-WPPA10 | 31.976 | 31.128 | 2.587 | 4 | OPC-WPPA15 | 26.934 | 26.503 | 1.526 | 5 | PPC-WPPA0 | 29.818 | 27.499 | 7.791 | 6 | PPC-WPPA5 | 27.091 | 24.996 | 7.720 | 7 | PPC-WPPA10 | 26.496 | 24.530 | 7.428 | 8 | PPC-WPPA15 | 23.066 | 21.539 | 6.677 |
|
|
Bold shows control mix.
|