Unconfined compressive strength test results.
| Aggregate type | Pressing methods | Optimum water content/% | Maximum unconfined compressive strength/MPa | Aggregate type | Pressing methods | Optimum water content/% | Maximum unconfined compressive strength/MPa |
| RCA | Vibratory compaction | 11.0 | 3.41 | RBA | Vibratory compaction | 16.5 | 2.31 | Static compaction | 3.49 | Static compaction | 2.46 |
| SRCA | Vibratory compaction | 10.5 | 4.08 | SRBA | Vibratory compaction | 15.5 | 3.13 | Static compaction | 4.25 | Static compaction | 3.41 |
| RCB | Vibratory compaction | 10.5 | 3.38 | RBB | Vibratory compaction | 16.0 | 2.18 | Static compaction | 3.39 | Static compaction | 2.34 |
| SRCB | Vibratory compaction | 10.0 | 4.01 | SRBB | Vibratory compaction | 15.0 | 3.06 | Static compaction | 4.07 | Static compaction | 3.19 |
|
|