Effect of Fiber Treatments on the Mechanical Properties of Sisal Fiber-Reinforced Concrete Composites

Table 9

Flexural strength test results.

Mix designationMean flexural strength (MPa)Relative strength gain compared to raw SFRC (%)

Control3.931
C0-03.950
C2–124.0793.285
C2–244.1605.336
C2–484.44012.403
C5–124.54915.180
C5–244.3379.795
C5–484.2597.843
C10–124.3369.775
C10–244.0372.219
C10–483.908−1.064