Research Article
Mechanical, Durability, and Gamma Ray Shielding Characteristics of Heavyweight Concrete Containing Serpentine Aggregates and Lead Waste Slag
| Mix code | Slump (mm) | Density (kg/m3) | Compressive strength (MPa) | Flexural strength (MPa) |
| F0C0 | 69 | 2622 | 38 | 4.14 | F0C25 | 71 | 2645 | 39.3 | 4.25 | F0C50 | 65 | 2668 | 38.1 | 3.95 | F0C100 | 62 | 2712 | 34.2 | 3.86 | F25C0 | 73 | 2659 | 43.1 | 4.2 | F25C25 | 74 | 2682 | 46.9 | 4.31 | F25C50 | 67 | 2707 | 44.3 | 4.01 | F25C100 | 66 | 2754 | 39.3 | 3.87 | F50C0 | 68 | 2707 | 41.2 | 4.03 | F50C25 | 69 | 2719 | 43.3 | 4.16 | F50C50 | 65 | 2752 | 42.3 | 3.93 | F50C100 | 64 | 2792 | 38.3 | 3.78 | F100C0 | 62 | 2782 | 37.1 | 4 | F100C25 | 63 | 2808 | 37 | 4.14 | F100C50 | 60 | 2829 | 36.9 | 3.81 | F100C100 | 59 | 3003 | 33.9 | 3.76 |
|
|