Experimental Torsional Capacity of Plain Concrete Beams Made from Crushed Clay Brick and Recycled Brick Concrete as Coarse Aggregate
Table 4
Mechanical properties of NSAC, VBAC, RSAC, and RBAC.
| Concrete type | Compressive strength (MPa) | SD | Tensile strength (MPa) | SD |
| NSAC18.9 | 19.8 | 0.267 | 2.2 | 0.063 | NSAC20.7 | 21.6 | 0.350 | 2.6 | 0.120 | NSAC22.4 | 23.5 | 0.398 | 2.9 | 0.087 | NSAC24.1 | 25.5 | 0.407 | 3.5 | 0.125 | VBAC18.9 | 17.8 | 0.594 | 1.8 | 0.103 | VBAC20.7 | 19.4 | 0.967 | 2.0 | 0.100 | VBAC22.4 | 21.0 | 0.822 | 2.2 | 0.161 | VBAC24.1 | 22.5 | 0.929 | 2.5 | 0.133 | RSAC18.9 | 17.7 | 0.386 | 1.8 | 0.016 | RSAC20.7 | 19.2 | 0.403 | 1.9 | 0.065 | RSAC22.4 | 20.7 | 0.368 | 2.2 | 0.069 | RSAC24.1 | 22.2 | 0.616 | 2.4 | 0.102 | RBAC18.9 | 17.4 | 0.785 | 1.7 | 0.056 | RBAC20.7 | 19.0 | 0.946 | 1.9 | 0.091 | RBAC22.4 | 20.4 | 1.208 | 2.1 | 0.132 | RBAC24.1 | 21.9 | 1.744 | 2.3 | 0.147 |
|
|
Note: SD: standard deviation.
|