Research Article
Effects of Thermal and Humidity Aging on the Interfacial Adhesion of Polyketone Fiber Reinforced Natural Rubber Composites
Table 3
Formulation of the RFL primer used in this study.
| | | Wet part (g) |
| | RF solution | | | Resorcinol | 16 | | Formaldehyde | 7 | | Sodium hydroxide | 1 | | Water | 200 | | Maturation: 25°C, 4 h | 224 |
| | Final dip solution | | | RF solution | 224 | | Latex | 160 | | Ammonium hydroxide | 5 | | Water | 120 | | Maturation: 25°C, 12 h | 509 |
|
|