Composition (weight fraction) of the check-point mixtures F1, F2, and F3 and corresponding measured (M) and predicted (P) values of hardness (HD), tensile strength (TS), elongation at break (EB), and rebound resilience (RS).

Wt. fractionF1F2F3

X1 (CC)0.3030.6770.860
X2 (PO)0.4380.6160.755
X3 (DV)0.0080.0150.009

PropertyPMPMPM

HD (Shore A)68.569.8 ± 0.776.278.4 ± 0.769.570.6 ± 0.7
RS (%)26.527.0 ± 0.025.025.0 ± 0.024.324.0 ± 0.0
EB (%)585.3668.3 ± 9.8470.5522.0 ± 19.2551.0526.7 ± 12.1
TR (MPa)10.4710.10 ± 0.38.929.32 ± 0.37.657.43 ± 0.2