Test results of HPCM with the recommend ratio.
| Results | Fluidity (s) | 1 day strength (MPa) | 3 days’ strength (MPa) | 7 days’ strength (MPa) | 28 days’ strength (MPa) | 60 days’ shrinkage ratio (%) | Flexural strength | Compressive strength | Flexural strength | Compressive strength | Flexural strength | Compressive strength | Flexural strength | Compressive strength |
| M1 | 13.4 | 1.55 | 17.33 | 4.90 | 31.20 | 5.50 | 44.83 | 8.35 | 61.59 | 0.1919 | M2 | 11.9 | 1.85 | 21.28 | 5.20 | 34.60 | 5.70 | 41.88 | 7.82 | 55.93 | 0.1883 | M3 | 12.7 | 1.30 | 17.03 | 5.10 | 32.63 | 5.8 | 42.98 | 7.51 | 54.53 | 0.1845 | Range | 10∼14 | — | — | — | — | ≥2 | 10∼30 | ≥4 | 20∼50 | −0.5∼0.5 |
|
|