Research Article
Fatigue Performance of SFPSC under Hot-Wet Environments and Cyclic Bending Loads
Table 2
Experimental conditions and results of group A∼D specimens.
| | Specimen number | Temperature, T (°C) | Relative humidity, H (%RH) | Stress level, SR = Pmax/Pu | Loading frequency, f (Hz) | Fatigue lives, Nf/cycles |
| | A1 | 23 | 78 | 0.70 | 10 | >2000000 | | A2 | >2000000 | | A3 | 825899 | | A4 | 0.75 | 293301 | | A5 | 328359 | | A6 | 349997 | | A7 | >2000000 | | A8 | 0.80 | 24099 | | A9 | 35677 | | A10 | 36071 | | B1 | 50 | 80 | 0.65 | 10 | >2000000 | | B2 | 1800031 | | B3 | 0.70 | 63470 | | B4 | 207900 | | B5 | 157413 | | B6 | 0.75 | 92486 | | B7 | 50936 | | C1 | 50 | 90 | 0.60 | 10 | >2000000 | | C2 | 1784833 | | C3 | 0.65 | 166591 | | C4 | 186596 | | C5 | 0.75 | 7940 | | C6 | 1960 | | D1 | 50 | 95 | 0.60 | 10 | >2000000 | | D2 | >2000000 | | D3 | 0.64 | 22236 | | D4 | 62746 | | D5 | 0.68 | 21355 | | D6 | 3647 | | D7 | 15173 |
|
|