Research Article

Performance of Coal Gangue-Based Cemented Backfill Material Modified by Water-Reducing Agents

Table 4

Performance indicators of CGCBM.

No.Performance index of rheologyBleeding rateCube compressive strength (MPa)
Slump (cm)Slump flow (cm) (Pa) (Pa·s)/%1 d3 d7 d14 d28 d

02030634.47.94.921.22.74.66.5
N12233563.62.31.30.41.53.05.08.3
N22340410.69.62.50.41.63.15.58.4
N323.543301.612.14.00.52.03.26.49.3
N42450252.612.74.40.52.03.15.88.7
N52762244.512.46.40.62.03.15.78.0
J12552384.71.700.31.83.36.38.5
J225.566319.35.900.42.23.67.28.7
J32764314.78.50.562.34.07.59.5
J427.543216.917.61.10.82.54.17.59.2
J525.583163.910.52.50.62.03.36.08.1