Compressive strength test results of steel fiber UHPC orthogonal test (MPa).
| Group number | W/B | Steel fiber (%) | Type of aggregate | Slag powder (%) | Quartz powder (%) | Silica powder (%) | Water reducing agent | Compressive strength (MPa) | 3 d | 7 d | 28 d |
| A1 | 0.18 | 0.5 | NS | 17 | 10 | 8 | 7.5 | 90.3 | 111.6 | 129.4 | A2 | 0.18 | 1.0 | QS | 17 | 10 | 8 | 9 | 90.1 | 110.8 | 137.1 | A3 | 0.18 | 1.5 | SS | 17 | 10 | 8 | 8.5 | 89.9 | 115.5 | 134.2 | A4 | 0.20 | 0.5 | QS | 17 | 10 | 8 | 9 | 76.8 | 105.4 | 121.5 | A5 | 0.20 | 1.0 | SS | 17 | 10 | 8 | 11 | 85.6 | 104.9 | 125.0 | A6 | 0.20 | 1.5 | NS | 17 | 10 | 8 | 10.5 | 87.6 | 108.8 | 127.6 | A7 | 0.22 | 0.5 | SS | 17 | 10 | 8 | 10.5 | 70.3 | 97.7 | 120.8 | A8 | 0.22 | 1.0 | NS | 17 | 10 | 8 | 11.5 | 69.3 | 98.5 | 123.2 | A9 | 0.22 | 1.5 | QS | 17 | 10 | 8 | 13 | 77.1 | 103.0 | 119.6 |
|
|