Research on Friction Stir Spot Welding Brazing Process and Properties of Dissimilar Metals DP590 and 6061
| Sample number | Rotating speed (r/min) | Residence time (s) | Pressing depth (mm) | Shear load (kN) |
| 1# | 1000 | 60 | 0.1 | 9.982 | 2# | 1000 | 90 | 0.2 | 13.239 | 3# | 1000 | 120 | 0.3 | 8.600 | 4# | 1200 | 60 | 0.2 | 6.681 | 5# | 1200 | 90 | 0.3 | 7.451 | 6# | 1200 | 120 | 0.1 | 7.835 | 7# | 1500 | 60 | 0.3 | 10.810 | 8# | 1500 | 90 | 0.2 | 8.959 | 9# | 1500 | 120 | 0.1 | 8.415 | Range | RA = 3.285 | RB = 1.603 | RC = 0.882 | — | Analysis | RA > RB > RC |
|
|