Measured responses of machining.

Exp. no.F (mm/min)V (volt)E (g/litre)MRR (mg/min)SN ratioFitsResidual

10.1510200.0027551.21330.0031112−0.0003612
20.2015250.0036648.73040.00322370.0004363
30.2520300.0028450.93360.0033362−0.0004961
40.3025350.0049946.03800.00344870.0015413
50.1515350.0031550.03380.0036200−0.0004700
60.2020200.0036248.82580.00360140.0000186
70.2525250.0024252.32370.0038450−0.0014250
80.3010300.0034549.24360.0038264−0.0003764
90.1520300.0054945.20860.00412890.0013611
100.2025350.0042547.43220.00424140.0000086
110.2510250.0043447.25020.00409160.0002484
120.3015200.0037348.56580.0042041−0.0004741
130.1520200.0041547.63900.0046377−0.0004877
140.2025350.0039248.13430.0046190−0.0006990
150.2510300.00661743.58680.00460040.0020166
160.3015250.0037448.54260.0045817−0.0008417