Table 2
Failure stresses in 4-point bending, diameters 78 cm and 85 cm.
| Specimen | AF(Ø78) | AF(Ø85) | σuH (MPa) | σu12 (MPa) | H (%) | σuH (MPa) | σu12 (MPa) | H (%) |
| 1 | 106.91 | 108.62 | 12.40 | 128.29 | 123.24 | 11.01 | 2 | 114.04 | 119.36 | 13.17 | 121.17 | 117.51 | 11.25 | 3 | 106.91 | 104.37 | 11.41 | 121.17 | 126.41 | 13.08 | 4 | 111.19 | 107.24 | 11.11 | 136.85 | 138.81 | 12.36 | 5 | 114.04 | 110.31 | 11.18 | 128.29 | 128.07 | 11.96 | 6 | 99.78 | 97.18 | 11.35 | 121.17 | 117.15 | 11.17 | 7 | 99.78 | 103.69 | 12.98 | 128.29 | 135.70 | 13.44 | 8 | 114.04 | 116.36 | 12.51 | 121.17 | 114.61 | 10.65 | 9 | 99.78 | 99.76 | 11.99 | 145.40 | 142.21 | 11.45 | 10 | 99.78 | 96.47 | 11.17 | 135.42 | 132.34 | 11.43 | 11 | 112.61 | 112.51 | 11.98 | 128.29 | 132.67 | 12.85 | 12 | 114.04 | 112.70 | 11.71 | 118.32 | 123.49 | 13.09 | Average | 107.74 | 107.38 | 11.91 | 127.82 | 127.68 | 11.98 | Standard deviation | 6.39 | 7.34 | 0.72 | 8.07 | 8.89 | 0.95 |
|
|