Study on Synthesis and Service Properties of Anticoagulant Ice Microcapsule Coating Material

Table 1

Properties of no. 90 A asphalt.

ItemsUnitSkill requirementTest resultsExperiment method

Penetration 100 g, 5 s, 25°C0.1 mm80∼10086T0604
Softening point TR&B°C≥4546.5T0606
Dynamic viscosity 60°CPa·s≥160187.1T0620
Ductility 5 cm/min, 10°Ccm≥45>100T0605
Ductility 5 cm/min, 15°Ccm≥100>100T0605
Wax content (distillation method)%≤2.21.7T0615
Flash point (COC)°C≥245264T0611
Solubility (trichloroethylene)%≥99.599.72T0607
Density, 15°Cg/cm3Measured record1.028T0603
After TFOTQuality change%≤±0.8−0.158T0609
Residual penetration ratio%≥5766.2T0604
Residual ductility, 10°Ccm≥814T0605