Research Article
Modification of Low-Density Slag Cementing Slurry with SiC Whiskers at High Temperature
Table 4
Formulations of the base slurry.
| Sample | Slag (g) | SiC whisker (g) | Activator (g) | Suspension agent (g) | Dispersant (g) | Water (g) |
| V | 100 | 0 | 5 | 0.4 | 0.5 | 75 | S1 | 99.5 | 0.5 | 5 | 0.4 | 0.5 | 75 | S2 | 99 | 1 | 5 | 0.4 | 0.5 | 75 | S3 | 98.5 | 1.5 | 5 | 0.4 | 0.5 | 75 | S4 | 98 | 2 | 5 | 0.4 | 0.5 | 75 |
|
|