Existing split tensile strength estimate models use different standard codes.
| Measured value | JSCE, 2007 [22]Fspt = 0.23Fc2/3 | ACI-363, 2008 [23]Fspt = 0.59√Fc | CSA, 2010 [24]Fspt = 0.67√Fc | NZS-3101, 2017 [25]Fspt = 0.54√Fc | Eurocode-2, 2007 [26]Fspt = 2.12Ln(1+0.1Fc) |
| 2.95 | 1.820 | 2.760 | 3.142 | 2.530 | 2.46 | 3.07 | 1.880 | 2.837 | 3.220 | 2.596 | 2.54 | 3.06 | 1.910 | 2.870 | 3.260 | 2.628 | 2.57 | 3.14 | 1.944 | 2.900 | 3.290 | 2.656 | 2.60 | 3.00 | 1.840 | 2.780 | 3.160 | 2.550 | 2.49 | 2.98 | 1.810 | 2.760 | 3.130 | 2.530 | 2.46 |
|
|