Research Article
Microstructure and Properties of Super-Ferritic Stainless Steels Used for Marine Construction after Fire Exposure
Table 2
The postfire mechanical properties of the SFSS.
| Samples | YS (MPa) | TY (MPa) | TE (%) |
| Before fire | 475 | 600 | 22.5 | 800°C × 0.5 h | 480 | 690 | 22.0 | 800°C × 1.0 h | 470 | 700 | 21.0 | 800°C × 2.0 h | 440 | 670 | 7.0 | 800°C × 4.0 h | 430 | 560 | 1.5 | 700°C × 0.5 h | 480 | 625 | 21.2 | 700°C × 1.0 h | 480 | 660 | 20.5 | 700°C × 2.0 h | 480 | 725 | 17.5 | 700°C × 3.0 h | 445 | 720 | 17.3 | 600°C × 0.5 h | 500 | 615 | 22.7 | 600°C × 1.0 h | 505 | 620 | 21.5 | 600°C × 2.0 h | 525 | 640 | 21.8 | 600°C × 3.0 h | 515 | 630 | 21.3 | 600°C × 4.0 h | 500 | 630 | 20.8 |
|
|