Research Article
Electropolishing of Additively Manufactured Ti-6Al-4V Surfaces in Nontoxic Electrolyte Solution
Table 1
Electropolishing parameters.
| | Parameters | Electrolyte 1 | Electrolyte 2 | Electrolyte 3 |
| | Triethanolamine | 180 ml | 180 ml | 180 ml | | Perchloric acid | 10 ml | — | — | | Sodium flouride (NaF) | 1.17% | 1.17% | 2% | | Ammonium flouride (NH4F) | 5% | 10% | 10% | | Oxalic acid | 16% | 16% | 16% | | Ethanol | 15 ml | 15 ml | 15 ml | | Current density | 0.2 Acm−2 | 0.2 Acm−2 | 0.2 Acm−2 | | Time | 30 min | 30 | 30 | | Temperature | 30.0 ± 2°C | 30.0 ± 2°C | 30.0 ± 2°C |
|
|