Research Article
A GPR-Based Test Study on the Influencing Factors of the Dielectric Constant of Cement-Stabilized Macadam Bases
Table 3
Relationship between the dielectric constant and strength of CSMB specimens.
| | Compaction degree (%) | Average compressive strength (MPa) | Average dielectric constant | Coefficient of determination | Fitted function |
| Fine | 92 | 3.41086 | 6.96593 | 0.98779 | | 94 | 3.57645 | 7.39290 | 0.89631 | | 96 | 4.28175 | 7.33488 | 0.90873 | | 98 | 4.76155 | 8.08176 | 0.95765 | | 100 | 5.69127 | 9.55040 | 0.98272 | |
| Coarse | 92 | 3.85619 | 7.53608 | 0.97117 | | 94 | 4.04465 | 7.89399 | 0.95968 | | 96 | 4.48533 | 8.24218 | 0.90271 | | 98 | 4.99977 | 8.98902 | 0.93418 | | 100 | 5.95318 | 10.00861 | 0.99453 | |
|
|