L16 orthogonal array experimental results.
| | Trial no. | TON (μs) | TOFF (μs) | I (A) | MRR (g/min) | SR (μm) |
| | 1 | 100 | 40 | 3 | 0.043 | 1.364 | | 2 | 100 | 50 | 6 | 0.169 | 3.621 | | 3 | 100 | 60 | 9 | 0.075 | 3.373 | | 4 | 100 | 70 | 12 | 0.104 | 3.81 | | 5 | 120 | 40 | 6 | 0.028 | 2.447 | | 6 | 120 | 50 | 3 | 0.194 | 3.614 | | 7 | 120 | 60 | 12 | 0.178 | 3.468 | | 8 | 120 | 70 | 9 | 0.135 | 2.268 | | 9 | 140 | 40 | 9 | 0.162 | 1.908 | | 10 | 140 | 50 | 12 | 0.069 | 2.669 | | 11 | 140 | 60 | 3 | 0.129 | 3.224 | | 12 | 140 | 70 | 6 | 0.019 | 1.916 | | 13 | 160 | 40 | 12 | 0.042 | 1.853 | | 14 | 160 | 50 | 9 | 0.107 | 3.831 | | 15 | 160 | 60 | 6 | 0.126 | 3.434 | | 16 | 160 | 70 | 3 | 0.055 | 3.518 |
|
|