Review Article

Enhancement of the Mechanical and Thermal Properties of Polypropylene and Nylon 6.6 Composite Blends

Table 2

Summary of three-point bending and hardness tests for pure PP and #16 samples.

Specimen namesPeak stress (MPa)Yield stress (MPa)Modulus (MPa)Hardness (MPA)MFI ratio

Pure PP31.825.5684.8133.01.0
1% #1631.426.7797.8191.00.95
2% #1635.528.5860.3172.40.98
3% #1625.925.1788.4146.61.15
4% #1629.425.8804.1187.10.83
5% #1624.322.5682.6150.51.31