Research Article
Experimental Study on Bonding Properties between Finishing Rolled Rebar and Grouting Material
Table 2
Test results of bond strength of specimens with different cover thicknesses.
| Number | C (mm) | D (mm) | c/d | Fu (kN) | τu (MPa) | τu,m(MPa) |
| A1-1 | 40 | 20 | 2.0 | 147.38 | 19.56 | 19.43 | A1-2 | 146.43 | 19.43 | A1-3 | 145.48 | 19.30 |
| A2-1 | 50 | 20 | 2.5 | 152.94 | 20.29 | 20.25 | A2-2 | 151.56 | 20.11 | A2-3 | 153.31 | 20.34 |
| A3-1 | 60 | 20 | 3.0 | 159.67 | 21.19 | 21.17 | A3-2 | 159.50 | 21.17 | A3-3 | 159.33 | 21.14 |
| A4-1 | 65 | 20 | 3.25 | 162.70 | 21.58 | 20.58 | A4-2 | 149.40 | 19.83 | A4-3 | 153.25 | 20.33 |
| B1-1 | 65 | 16 | 4.06 | 160.94 | 26.69 | 25.35 | B1-2 | 130.02 | 21.56 | B1-3 | 167.68 | 27.80 |
| B2-1 | 65 | 18 | 3.61 | 125.63 | 18.53 | 21.02 | B2-2 | 148.00 | 21.83 | B2-3 | 153.98 | 22.71 |
| B3-1 | 65 | 25 | 2.6 | 146.43 | 15.54 | 16.98 | B3-2 | 166.17 | 17.64 | B3-3 | 167.40 | 17.77 |
|
|