Research Article
Introduction to the New Copolymer of Chloroprene and Acrylonitrile with Differentiated Properties
Table 3
Mooney viscosity, scorch, and cure characteristics of acrylonitrile-chloroprene rubber (NCR), chloroprene rubber (CR), and nitrile rubber (NBR).
| | NCR | CR | NBR |
| Mooney viscosity of compounds (ML1+4), 100°C | 55 | 70 | 55 | Scorch time (, min), 125°C | 17.7 | 9.4 | 16.4 | Rheometer (ARR) data, 170°C, 30 mins | | | | Minimum torque (, N·m) | 0.1 | 0.2 | 0.1 | Maximum torque (, N·m) | 1.6 | 2.2 | 1.1 | (N·m) | 1.5 | 2.0 | 1.1 | (min) | 3.8 | 2.2 | 1.7 | Time corresponds to 10% cure (, min) | 3.5 | 2.1 | 1.5 | Time corresponds to 90% cure (, min) | 9.7 | 5.6 | 4.7 | Cure rate index (min-1) | 16.9 | 29.4 | 33.3 |
|
|