Effect of Printing Layer Thickness and Postprinting Conditions on the Flexural Strength and Hardness of a 3D-Printed Resin
Table 2
The means and standard deviations of the Vickers hardness and flexural strength values found for the 3D-printed material.
Postprinting treatment conditions
3D printing thickness
20
50
100
FS ()
VHN ()
FS ()
VHN ()
FS ()
VHN ()
Dry storage (control)
91.51 (10.05)a
13.23 (0.48)a
94.40 (9.61)a
16.23 (0.22)a
91.51 (10.05)a
9.31 (0.22)a
WS for 24 h
68.38 (9.02)b
10.68 (1.67)a
88.25 (8.83)b
16.63 (0.10)a
68.38 (9.02)b
12.71 (2.97)a
WS for 1 month
64.37 (7.43)b
14.86 (1.85)a
77.67 (9.13)bc
16.38 (0.35)a
64.37 (7.43)b
13.90 (0.45)b
LC 5 min
80.80 (8.72)ab
14.33 (0.08)b
83.76 (10.44)c
16.63 (0.51)b
80.80 (8.72)ab
12.45 (1.41)a
LC 15 min
82.80 (9.09)ab
15.21 (0.12)a
91.02 (4.80)ab
16.20 (1.10)b
82.80 (9.09)ab
12.93 (0.42)ab
HC 5 min
71.32 (4.46)bc
13.46 (0.34)c
83.47 (12.08)bd
17.06 (0.30)c
71.32 (4.46)bc
17.95 (1.09)c
HC 15 min
64.83 (9.07)bd
12.41 (0.35)a
88.86 (8.03)bd
17.66 (0.81)d
64.83 (9.07)bd
14.88 (0.31)ad
FS: flexural strength; VHN: Vickers hardness. Same superscripted lowercase letters indicate groups not statistically significantly different when compared by Tukey’s multiple comparison post hoc analysis ().