Parameters of pull-out specimens with deformed rebar.

References No.Specimen size (mm)Corrosion level (%)
(MPa)

(mm)

(mm)
No. of specimens (mm)Stirrup confinementReinforcement positionTest environmentReinforcement type

[3]100×100×1000–9.9522.1312441480NoCenterDirect currentRibbed bars
[4]100×100×1000–9.7222.1312441480NoCenterAccelerated corrosionRibbed bars
[5]100×100×1000–813.98, 21.1, 23.631244215dNoCenterElectro-migrationRibbed bars
[6]150×150×1500–4.6662.7, 73.412693960NoCenterCurrent density of 0.25mA/cm2Ribbed bars
[7]120×120×1200–2030.91254205dEach halfCenterCurrent density of 200uA/cm2Ribbed bars
[8]152×254×2800–79.74301263.5No102YesSideDirect current (0.4 A)Ribbed bars
[9]140×140×1800–952.12060244dEach halfCenterDirect current (0–2 A)Ribbed bars
[14]200×200×2000–14.4520.7, 44.418914080YesCenterCurrent density of 150μA/cm2Ribbed bars
[16]140×140×1800–9.0254.152060244dEach halfCenterCurrent density of 1.214mA/cm2Ribbed bars
[17]100×100×2000–2.370938.316, 2042, 40205dEach halfCenterElectro-migration (DC voltage of 60V)Ribbed bars
[18]150×150×1500–9.0624.8118, 20, 22301750NoSideAccelerated corrosionRibbed bars
[20]100×100×1500–11.833.51642550NoCenterAccelerated corrosionRibbed bars
[22]140×140×1800–6.152.12060244dEach halfCenterDirect current (0–2 A)Ribbed bars
[23]150×150×1500–5.9541.9186612100Each halfCenterElectro-migration and wetting-drying cycleRibbed bars
[24]140×140×1800–27.950.82060314dEach halfCenterDirect current (0–2 A)Ribbed bars
[25]150×150×1500–2.321, 322562.5304dNoCenterAccelerated corrosionRibbed bars
[26]120×120×1200–0.830.11254125dNoCenterCurrent density of 0.25mA/cm2Ribbed bars
180×180×1800–4.530.11881125dNoCenterCurrent density of 0.25mA/cm2Ribbed bars
[27]140×140×1800–15.2731.42060203dYesCenterCurrent density of 0.01–0.02mA/mm2Ribbed bars
[28]150×150×1500–8.9523, 511415, 30, 459050NoSideDirect current (0–5 A)Ribbed bars
[29]140×140×1800–20642060214dYesCenterMaximum of 0.1 A per specimenRibbed bars
[30]150×150×1500–12-126964dNoCenterDirect current (17.5–59mA)Ribbed bars
[31]150×150×2000–2.528.31368.5213dNoCenterAccelerated corrosionRibbed bars
150×150×2000–8.828.313684039NoCenter Output of 24 V DC and 12 ARibbed bars
[32]150×150×1500–6.692912691370NoCenterCurrent density of 100μA/cm2Ribbed bars
[33]104×104×1040–2424.7, 33, 42.11345.5678Each halfSideMaximum of 1 A per specimenRibbed bars
[34]10d×10d×10d0–4.930.112, 184.5d245dNoCenterCurrent density of 0.25mA/cm2Ribbed bars
[35]160×160×2500–15.935.82035, 45, 5527200YesSideDirect current (0–1 A)Ribbed bars
[36]150×150×1500–9.824.83, 26.51, 25.04206545100NoCenterDirect current (0–2 A)Ribbed bars
[37]150×250×3000-14.6533203516100YesSideCurrent density of 500μA/cm2Ribbed bars
[38]175×175×3500–5.19-19781175NoCenterDirect current (0.15 A)Ribbed bars
[39]150×150×1500–9.0624.8118, 20, 223034100NoSideDirect currentRibbed bars
[40]150×250×3000–10.1950203543100YesSideCurrent density of 400–600μA/cm2Ribbed bars