| Weight Loss, % | WHF (C) | MW0 (C) | MW15 (C) | MW30 (C) | MW40 (C) | MW50 (C) |
| 5 | 216.4 | 293.0 | 273.3 | 278.5 | 267.0 | 267.1 | 10 | 267.0 | 366.6 | 319.3 | 319.8 | 302.9 | 302.8 | 20 | 296.8 | 459.6 | 447.3 | 431.9 | 385.2 | 366.5 | 30 | 312.0 | 472.5 | 466.9 | 468.5 | 461.5 | 462.3 | 40 | 324.5 | 479.8 | 475.9 | 479.5 | 473.7 | 475.9 | 50 | 340.5 | 486.0 | 482.9 | 486.9 | 481.5 | 484.4 | 60 | 430.4 | 492.1 | 488.6 | 493.9 | 488.9 | 492.0 | 70 | 544.5 | 499.0 | 496.8 | 502.7 | 499.0 | 502.5 |
|
|