Research Article
Cracking Behaviour of Alkali-Activated Aluminosilicate Beams Reinforced with Glass and Basalt Fibre-Reinforced Polymer Bars under Cyclic Load
Table 7
Behaviour of cracks under cyclic and static load.
| Specimen ID | First crack load | Ultimate load | Total no of cracks-first | Total no of cracks-ultimate | Crack propagation-first | Crack propagation-ultimate | Spacing of cracks-first | Spacing of cracks-ultimate | Avg. crack width-first | Avg. crack width-ultimate | (KN) | (KN) | (Nos) | (Nos) | (mm) | (mm) | (mm) | (mm) | (mm) | (mm) |
| BRGC-C | 6 | 34.80 | 7 | 18 | 70 | 127 | 110 | 95 | 0.02 | 0.2 | GRGC-C | 6 | 27.30 | 6 | 17 | 95 | 137 | 120 | 120 | 0.08 | 0.38 | SRCC-C | 15 | 44.55 | 6 | 15 | 72 | 106 | 153 | 85 | 0.03 | 0.08 | BRGC-S | 9 | 33.45 | 9 | 16 | 105 | 130 | 128 | 89 | 0.2 | 0.56 | GRGC-S | 6 | 32.4 | 6 | 13 | 135 | 153 | 197 | 73 | 0.24 | 0.78 | SRCC-S | 15 | 49.80 | 5 | 15 | 48 | 116 | 115 | 71 | 0.09 | 0.30 |
|
|