The response surface experimental results.
| | No. | Cutting speed (m/min) | Feed rate f (mm/r) | Cutting depth ap (mm) | Surface roughness Ra (μm) | Surface microhardness HV |
| | 1 | 60 | 0.12 | 0.2 | 1.36 | 455 | | 2 | 30 | 0.06 | 0.3 | 0.79 | 435 | | 3 | 60 | 0.12 | 0.2 | 1.28 | 460 | | 4 | 90 | 0.06 | 0.1 | 0.7 | 438 | | 5 | 30 | 0.06 | 0.1 | 0.68 | 440 | | 6 | 90 | 0.18 | 0.3 | 2.51 | 449 | | 7 | 60 | 0.18 | 0.2 | 2.17 | 450 | | 8 | 60 | 0.06 | 0.2 | 0.74 | 456 | | 9 | 90 | 0.18 | 0.1 | 1.81 | 412 | | 10 | 60 | 0.12 | 0.1 | 1.35 | 440 | | 11 | 60 | 0.12 | 0.2 | 1.32 | 458 | | 12 | 60 | 0.12 | 0.2 | 1.2 | 449 | | 13 | 90 | 0.06 | 0.3 | 0.83 | 421 | | 14 | 30 | 0.12 | 0.2 | 1.58 | 426 | | 15 | 90 | 0.12 | 0.2 | 1.37 | 420 | | 16 | 30 | 0.18 | 0.3 | 2.32 | 480 | | 17 | 60 | 0.12 | 0.2 | 1.45 | 452 | | 18 | 60 | 0.12 | 0.3 | 1.53 | 468 | | 19 | 60 | 0.12 | 0.2 | 1.21 | 448 | | 20 | 30 | 0.18 | 0.1 | 2.27 | 426 |
|
|