Research Article
Experimental Study on Chloride Stress Corrosion Cracking Sensitivity of 316L Stainless Steel
Table 6
Main mechanical properties of 316L stainless steel at different temperatures.
| | T (°C) | Tensile strength σb (MPa) | Reduction of area ψ (%) | Elongation δ5 (%) | Fracture time (h) |
| | 25 | 558.0 | 84.8 | 56.2 | 36.3 | | 45 | 551.0 | 82.7 | 54.1 | 35.4 | | 65 | 532.0 | 83.7 | 49.5 | 35.1 | | 85 | 517.0 | 77.6 | 45.9 | 32.9 |
|
|