Research Article
Mechanical and Durability Characteristics of TiO2 and Al2O3 Nanoparticles with Sisal Fibers
Table 1
Mix proportions of concrete specimens.
| Mix ID | Cement (kg/m3) | Fine aggregate (kg/m3) | Coarse aggregate (kg/m3) | Water content (kg/m3) | TiO2 nanoparticles (kg/m3) | Al2O3 nanoparticles (kg/m3) | Sisal fibers (kg/m3) |
| CC | 435 | 672 | 1179 | 172 | 0 | 0 | 0 | CC-1 | 413.25 | 672 | 1179 | 172 | 13.05 | 0 | 8.7 | CC-2 | 408.9 | 672 | 1179 | 172 | 17.4 | 0 | 8.7 | CC-3 | 413.25 | 672 | 1179 | 172 | 0 | 13.05 | 8.7 | CC-4 | 408.9 | 672 | 1179 | 172 | 0 | 17.4 | 8.7 | CC-5 | 400.2 | 672 | 1179 | 172 | 13.05 | 13.05 | 8.7 | CC-6 | 391.5 | 672 | 1179 | 172 | 17.4 | 17.4 | 8.7 |
|
|