Sl. no.Type of RMwt% of RM content (%)Injection pressure (MPa)Tensile strength (MPa)Impact strength (J)S/N ratio
Tensile strengthImpact strength

1SiC58054.661.9634.7531.73
2SiC59050.661.9734.0932.59
3SiC510048.452.0033.7133.40
4SiC158045.331.8833.1333.56
5SiC159046.331.8233.3232.79
6SiC1510046.331.8533.3232.80
7SiC258053.851.8734.6233.17
8SiC259055.851.9634.9434.58
9SiC2510049.851.9633.9534.58
10B4C58045.654.033.1930.53
11B4C59044.654.033.0031.03
12B4C510043.654.132.8031.55
13B4C158041.333.232.3331.28
14B4C159043.333.3332.7431.73
15B4C1510042.333.032.5332.80
16B4C258046.852.233.4132.78
17B4C259047.852.133.6032.82
18B4C2510041.852.032.4332.58