Research Article
The Forecasting of Corrosion Damage of Structural Materials during Dry Long-Term Storage of RD BN-350 SNF with CC-19 SFA
Table 4
The corrosion indicators of the samples in argon medium during the experiment.
| Sample | Test temperature, °С | | | | The depth of corrosion during the experiment, μm | (g/m2h) | (g/m2h) | (mm/year) |
| Irradiated FA jacket | 550 | 0.000741 | 0.003459 | 0.003787 | 3.05 | Nonirradiated FA jacket | 0.000468 | 0.002182 | 0.002389 | 1.92 | Nonirradiated fuel element cladding | 0.000530 | 0.002600 | 0.002840 | 2.29 |
| Irradiated FA jacket | 400 | 0.000100 | 0.000490 | 0.000537 | 0.43 | Nonirradiated FA jacket | 0.000040 | 0.000194 | 0.000212 | 0.17 | Nonirradiated fuel element cladding | 0.000040 | 0.000220 | 0.000240 | 0.19 |
| Irradiated FA jacket | 300 | 0.000064 | 0.000312 | 0.000341 | 0.27 | Nonirradiated FA jacket | 0.000039 | 0.000190 | 0.000210 | 0.17 | Nonirradiated fuel element cladding | 0.000030 | 0.000170 | 0.000180 | 0.15 |
|
|