Research Article
Study on the Microstructure and Mechanical Properties of As-Extruded AZ Magnesium Alloys by Micro-Adding La Rare-Earth Element
Table 3
EDS analysis results of precipitates in as-extruded AZ-0.3La alloys (in %).
| Alloy | Precipitate | Elements | Mg | Al | La | Zn | Mn | Total |
| AZ01-0.3La | A(Mg-La-Mn) | 90.1 | — | 8.31 | — | 1.59 | 100 | AZ31-0.3La | B(Al11La3) | 42.8 | 44.3 | 12.7 | — | 0.02 | 100 | C(Al11La3) | 78.8 | 16.8 | 4.40 | — | — | 100 | AZ61-0.3La | D(Al11La3) | 30.9 | 51.9 | 14.4 | 2.80 | — | 100 | E(Al11La3) | 12.0 | 66.1 | 18.4 | 3.50 | — | 100 | AZ80-0.3La | F(Mg17Al12) | 92.6 | 6.56 | 0.84 | — | — | 100 | G(Al11La3) | 25.5 | 57.9 | 13.3 | 3.30 | — | 100 |
|
|