Research Article
Evaluation of Fatigue Life of CRM-Reinforced SMA and Its Relationship to Dynamic Stiffness
Table 1
Properties of base binder grade 80/100 penetration.
| Test properties | Value | Standard test |
| Viscosity at 135°C (Pas) | 0.65 | ASTM D4402 |
G*/ at 64°C (kPa) | 1.35 | ASTM D4-P246 | Ductility at 25°C | >100 | ASTM D113 | Softening point at 25°C | 47 | ASTM D36 | Penetration at 25°C | 88 | ASTM D5 | Flash point (°C) | 300 | ASTM D9 | Fire point °C | 317 | ASTM D9 | RTFOT aged G*/ at 64°C (kPa) | 6.022 | ASTM D2872 | PAV aged at 25°C (kPa) | 3122.5 | ASTM D6521 |
|
|