The Influence of Polymerization Type and Reinforcement Method on Flexural Strength of Acrylic Resin
Table 2
Flexural strength means and standard deviations (MPa) for different polymerization and reinforcement methods.
Groups
Mean (SD)
Self-polymerized (SP)
Heat-polymerized (HP)
Unidirectional glass fiber (Uni)
241.71 (67.77)Aa
215.14 (67.60)Aba
Short glass fiber (Short)
156.31 (28.76)BCDa
198.44 (95.27)ABCa
Unidirectional and short glass fiber (Uni-Short)
221.06 (71.97)Aa
189.56 (92.27)ABCa
Industrialized glass fiber (Ind)
215.61 (46.59)Aba
268.93 (105.65)Aa
Thermoplastic resin (Tpl)
132.51 (20.21)CDa
161.32 (62.51)CDa
Steel wire (SW)
190.51 (31.49)ABCa
106.69 (28.7)CDb
Control
101.47 (19.79)Da
93.39 (39.61)Da
(i) Different capital letters mean significant differences within the same acrylic resin (vertical comparison only). (ii) Different lowercase letters mean significant differences within the same reinforcement method (horizontal comparison only).