Mechanical properties of the prepared composites.
| Sl. number | Material | Hardness value (BHN) | Yield strength (MPa) | Ultimate tensile strength (MPa) | Elongation (%) |
| (1) | Sample-I | 43 | 67 | 131 | 13 | (2) | Sample-II | 63 | 115 | 154 | 8.13 | (3) | Sample-III | 75 | 133 | 165 | 6.10 |
|
|