Research Article

Tear Strength Analysis of MDX4-4210 and A-2186 Silicones with Different Intrinsic Pigments Incorporated by Mechanical and Industrial Methods

Table 3

Mean values ± standard deviation (SD) (N/mm) of tear strength values comparing aged MDX4-4210 and A-2186 silicones, based on same pigmentation.

Manufacturing methodPigmentSiliconeAged groups value
Mean ± SD

MechanicalBronzeMDX4-421041.16 ± 4.31<0.001
A-218672.12 ± 11.17
BlackMDX4-421041.25 ± 3.82<0.001
A-218664.87 ± 13.91
PinkMDX4-421031.65 ± 2.05<0.001
A-218665.56 ± 12.83

IndustrialBronzeMDX4-421037.82 ± 3.52<0.001
A-218673.10 ± 11.56
BlackMDX4-421042.53 ± 6.66<0.001
A-218665.17 ± 11.85
PinkMDX4-421031.06 ± 4.11<0.001
A-218670.46 ± 6.07

Statistically significant difference (, Tukey).