Research Article

Chemo-Mechanical Approach to Improve Repair Bond Strength of Denture Teeth

Table 2

Mean shear bond strength ± SD (MPa) and significance of repaired specimens with different surface treatments at 0 and 5,000 thermal cycles.

Treated sideGroup0 thermal cycles, mean ± SD5,000 thermal cycles, mean ± SD

No treatmentControl9.78 ± 0.816.97 ± 0.50

BaseB-AB17.02 ± 1.00a15.74 ± 0.72a
B-AB + SCA21.59 ± 1.1018.61 ± 0.76b

ToothT-AB15.81 ± 0.60a14.85 ± 0.54c
T-AB + SCA18.00 ± 1.10a,b15.19 ± 0.71a,c

Base and toothBT-AB18.98 ± 0.60b,A18.44 ± 0.76b,A
BT-AB + SCA23.91 ± 0.9620.05 ± 0.49

Groups with similar letters are not significantly different from each other. Vertically identical superscripted small letters denote no significant differences among groups . Horizontally identical superscripted capital letters denote no significant difference after thermal cycling within the surface treatment group .