Mean and standard deviation (±sd) of bond strength (in MPa) for the study groups and evaluated thirds.

Root regionControl GroupExperimental groups
SILBLASTBLAST + SILPERPER + SIL
Mean (±sd)Mean (±sd)Mean (±sd)Mean (±sd)Mean (±sd)Mean (±sd)

Cervical9.5 (2.4)Aa12.6 (3.3)BCa10.3 (3.5)ACa14.2 (3.2)Ba9.4 (2.4)Aa13.8 (4.3)Ba<0.001
Medium6.0 (2.0)Ab10.2 (3.2)Bb9.8 (3.0)Ba10.5 (2.0)Bb6.7 (2.2)Ab11.8 (4.9)Bab<0.001
Apical4.7 (2.1)Ab8.8 (3.0)Bb5.6 (3.7)Ab9.8 (2.3)Bb5.2 (2.0)Ac9.1 (3.9)Bb<0.001
Total6.5 (2.9)A10.5 (3.5)B8.6 (4.0)C11.5 (3.2)B7.1 (2.8)AC11.6 (4.6)B<0.001

was calculated using the ANOVA test followed by Tukey’s test. Different upper-case letters represent statistically significant differences ( < 0.05) between treatment types in the same third root. Different lowercase letters represent statistically significant differences ( < 0.05) between the third roots with the same treatment group.